On an equipment case, the shell is packaging and the insert is the product protection. Buyers spend weeks on shell material and colour and then accept whatever foam the factory proposes. That is backwards: the insert decides whether the item arrives intact, and it is where reorders go wrong when a supplier quietly changes grade.
| Insert type | Cavity tolerance | Best fit |
|---|---|---|
| Die-cut PE or EPE foam | ±2–3 mm | Instruments, tools, electronics; high volume, one layout |
| CNC-milled foam | ±1.5 mm | Low volume, deep cavities, layouts that will change |
| Moulded flocked EVA | ±0.5 mm | Visible presentation, daily handling, retail display |
Tolerances are working figures from our own sampling. The number that matters is the one written on your drawing, tested on a dropped case.
Why the insert is the engineering, not the accessory
A case has one job: keep the product inside it working. The EVA shell does that by being stiff, and stiffness without a insert only means the product bounces around inside a rigid box. Everything that happens on the way — the courier's conveyor, the pallet dropped from a tail lift, the warehouse stack — arrives at the product through the insert. Get the insert right and a modest shell is enough. Get it wrong and a good shell just keeps the pieces together.
It is also the part of the case that is easiest to change without telling the buyer. Foam is bought by the sheet, grade names are not standardised, and a factory under cost pressure can move from 30 kg/m³ to 25 without anyone noticing at inspection, because both look like white foam. Six months later the cavity has gone slack and the instrument rattles. That is the failure mode this article is about.
Foam is not one material, and the names are not standard
Four families cover almost everything shipped in a moulded case. What separates them is behaviour under load, under humidity, and over time:
| Material | Typical density | Behaviour | Where it goes wrong |
|---|---|---|---|
| PU foam (polyurethane) | 20–35 kg/m³ | Soft, cheap, cuts cleanly | Hydrolyses in storage; crumbles at cut edges after a year or more |
| PE foam (polyethylene) | 25–45 kg/m³ | Closed cell, resilient, moisture resistant | Less conforming on complex shapes; needs a sharper layout |
| EPE (expanded PE) | 20–40 kg/m³ | Bead structure, very good repeated impact | Cuts rougher; visible bead texture, not a display finish |
| EVA sheet | 60–80 kg/m³ | Firm, dimensionally stable, thermoformable | Too stiff alone for fragile goods; used as a structural layer |
The practical rule: polyurethane is what you get if you do not specify, and it is the one that fails in the warehouse. For anything that might sit in stock for a year, name PE or EPE on the drawing, or accept that the foam has a shelf life.
Density follows the weight of the item, not a house habit. Under 500 g, 25–30 kg/m³ is enough and stays soft. One to three kilos needs 30–45. Above that, or where the case itself will be stacked, the insert needs a denser grade or an EVA sheet layer behind the cavity. A foam that is too soft lets the item settle, the cavity walls wear into a taper, and by the third shipment the fit is gone. A foam that is too hard stops absorbing and starts transmitting: the case survives the drop and the product inside does not.
Three ways to make a cavity, and what each costs
Die-cut foam
A steel-rule die is made once to the layout, then pressed through stacked foam sheets. The die is the tooling; the foam is the consumable. Per unit it is the cheapest of the three at volume, and it allows a multi-layer build: a firm base layer, the cavity layer, and a thin top layer that closes over the product when the case is shut. Tolerance is ±2–3 mm, because the blade compresses the foam as it cuts and the foam relaxes afterwards.
CNC-milled foam
No die. A block of foam is cut to the drawing by a machining head, which suits low volumes, deep cavities and layouts that are still moving. Tolerance is better, around ±1.5 mm, and there is no tooling cost, so it is the right answer for a pilot run of 100 or a design that will be revised. Per unit it costs more than die-cutting and the surface is slightly rougher.
Moulded flocked EVA
Here the cavity is formed in a mould rather than cut out of a sheet. An EVA sheet is heated, vacuum-formed over a tool, then the inside is coated with adhesive and flocked — short nylon fibres blown onto the surface so they stand up, giving the velvety finish. The result is a shell-within-a-shell: firm, dimensionally stable to about ±0.5 mm, no loose foam dust, and it wipes clean. It is the right choice when the case is opened in front of a customer.
The cost structure differs enough to matter. Die-cut pays once for a die and little per unit; CNC pays nothing up front and more per unit; flocked EVA pays for a mould and for a slower forming cycle, so it only makes sense from a few hundred pieces upward, and it commits you to a shape. Mixing them is common and sensible: flocked EVA for the visible top tray, die-cut PE underneath where nobody looks.
What to put on the drawing
An insert drawing that can be quoted and inspected has seven things on it. Most buyers send a photo of the product and a sketch of a rectangle:
| Item | What to state | Why it matters |
|---|---|---|
| Material and density | PE 30 kg/m³, or EPE, or EVA 70 kg/m³ | "Sponge foam" is not a material; it is an invitation to substitute |
| Layer build | Base 20 mm + cavity 40 mm + top 10 mm | Decides whether the product is held from below, above, or both |
| Cavity tolerance | ±2–3 mm, with the fit direction named | A cavity cannot be both snug and easy to pull out |
| Clearance | 1–2 mm per side around the product | Snug without being an interference fit |
| Finger lifts | Position and size, typically 25–30 mm wide | Nobody can remove a flush-fit instrument without one |
| Surface finish | Raw foam, or flocked, or fabric-lined | Decides whether dust is an issue and how it is cleaned |
| Test | Drop height, faces, and what counts as a fail | Without this, "protective" is an opinion |
Two of those rows cause most of the arguments. Clearance: specify a cavity smaller than the product to "hold it tight" and the foam loses that argument on the first drop — the item compresses the foam once and then sits loose for the rest of its life. Finger lifts: skip them and the user pries the instrument out with a screwdriver, which damages both.
The test line is the one buyers leave blank and then argue about. A workable default: 1.2 m drop onto a rigid floor, all six faces plus one edge and one corner, case closed and latched, product installed, and a pass means the product still functions and shows no deformation. That is ISTA 1A territory; if the case ships in a retail carton or on a pallet, the relevant sequence moves to ISTA 3A. If the product is genuinely fragile, the drop height goes up and the cavity design changes — not just the foam density.
Six questions before you accept the insert quotation
| Ask | Good answer | Answer that should worry you |
|---|---|---|
| Which foam, at what density? | A named material and a number | "High quality sponge" |
| Die-cut, CNC or moulded? | Named, with the reason for the choice | "Whatever is cheaper" |
| Is the die a separate line? | Yes, with the cost stated and ownership confirmed | Tooling absorbed into the unit price |
| What is the cavity tolerance? | A number in millimetres | Silence |
| Has one been drop tested? | A height, a face count, and a result | "It is very safe, we have done this for years" |
| What happens on a reorder? | Same foam grade, same die, grade stated on the PO | "Standard packing, same as last time" |
The last question is not pedantry. The insert is the component most likely to change between orders, because it is the cheapest thing to substitute and the hardest thing to see. Put the foam grade, the density and the die number on the purchase order, not just on the first quotation, and check one insert against the approved sample at every inspection.
Where the case sits inside a larger programme — a product that ships with a tool, a spare and a manual — the insert also decides the packing sequence, and therefore the carton dimensions and the freight. That chain is covered in how packaging changes your freight cost.
Frequently asked
Is die-cut foam or flocked EVA better for an equipment case?
Steel-rule die cutting and CNC routing solve different problems, and the choice follows the cavity depth and the number of design changes you expect Die-cut foam is cheap per unit once the die exists, holds a precise cavity, and lets the product sit in a recognisable cut-out, which is why it is the default for instruments, tools and electronics. Flocked EVA is a moulded shell with a fabric-flocked surface, so the cavity is formed rather than cut: it looks finished, does not shed, wipes clean and survives years of opening. It costs more to tool and is worth it when the case is on display or the product is handled daily. Many programmes use both: flocked EVA for the visible top tray, die-cut foam underneath.
What foam density should a protective insert use?
Match density to the weight of the item, not to a habit. For a light instrument under about 500 g, 25 to 30 kg per cubic metre polyethylene foam is enough and stays soft. For 1 to 3 kg, 30 to 45 kg per cubic metre holds shape without collapsing. Above that, or where the case will be stacked in a warehouse, the insert needs a denser grade or a structural layer such as EVA sheet at 60 to 80 kg per cubic metre. A foam that is too soft lets the item settle and the cavity walls wear into a taper; too hard and the foam transmits the impact rather than absorbing it.
Why does the foam in some cases turn to dust after a year?
Because cheap polyurethane foam hydrolyses: it absorbs moisture from the air, the cell walls break down and the foam crumbles, usually starting at the exposed cut edges. The failure shows up in stock, not in the factory, which is why it is discovered by a customer. Polyethylene and expanded polyethylene foams are far more resistant and are the safer choice for goods that may sit in a warehouse or a retail back room for a year or more. If the programme uses PU foam, ask what grade it is and how it was stored, and expect a shorter shelf life.
What tolerance can I expect on a die-cut cavity?
Die-cut foam typically holds plus or minus 2 to 3 mm, because the blade compresses the foam as it cuts and the foam relaxes afterwards. CNC-milled foam holds about plus or minus 1.5 mm; a moulded EVA shell holds about plus or minus 0.5 mm on the formed cavity. Design the cavity 1 to 2 mm larger than the product on each side so the fit is snug without being an interference fit, and never specify a cavity smaller than the product to stop movement: the foam loses that argument the first time the case is dropped.
Who owns the die for a die-cut insert?
Whoever pays for it, and that should be stated in writing. A steel-rule die for an insert is a one-off cost per layout, typically a few hundred US dollars, and it is reusable on every reorder of the same layout. For a custom insert, buyers normally pay for the die and keep it; the factory stores it. If the supplier folds the die cost into the unit price instead, you are paying for it on every reorder. Ask for the die cost as a separate line and for a written statement that the die stays with your programme, including if you move the work.
Send the product, its drawing and the way it will be shipped. The insert design and the drop test come back with the quote.
Equipment cases run from 500 pcs; standard bag MOQ 1,000 pcs per style and colour. Sampling 7–15 days, mass production 35–50 days, T/T 30/70.
Related reading
- Equipment cases — the case programmes this insert work sits inside.
- Moulded EVA cases — how the shell itself is built and what the mould costs.
- How packaging changes your freight cost — why the insert decides the carton and the freight bill.
- Who pays for bag tooling and dies — die ownership and what happens when you move the work.
- Bag inspection checklist — where the insert check belongs in a pre-shipment inspection.